Related austenitic stainless steel grades

Introduction

The table is intended to relate former BS, En, German and Swedish grade designations to the current EN steel numbers, AISI grades ('grades' in (brackets) are not a true AISI grades) and UNS (Unified Numbering System) numbers. The table is based on the 'wrought' ie long products (bars etc), flat products (plates etc) steel numbers published in EN 10088 and related standards. Castings products use different compositions and so have their own steel numbers in EN 10283. The related castings grades in both EN 10283 and BS 3100 are included in the table.

The 'Composition Guide' is intended to represent the composition only. This does not show the specified or typical compositions of commercially available steels. Specified ranges for the wrought European grades can be found in either the BS EN 10088-2 or BS EN10088-3 tables. Most of the specified ranges for the 'BS' grades can be found in the BS 1449 or BS 970 tables. The castings grades specified ranges can be found in the BS EN 10283 or BS 3100 tables. Direct links to tables giving the specified range is available for the grades with underlines in the table. Just click on the number.

As an alternative to scanning down the list try the 'find' facility on your keyboard, using the 'Ctrl' and 'F' keys together. Type in the term you are looking for in the dialog box that then appears.

These are comparisons only and cannot be assumed to be direct equivalent grades. The data given is not intended to replace that shown in individual standards to which reference should always be made.

Grades table

EN (10088) Common Names BS (Wrought) AISI UNS En German SS EN (10283) BS (Cast) Composition Guide
. . . . . . . . . . C Cr Ni Mo Others
1.4301 - 304S31 304 S30400 58E X5CrNi18-10 2333 1.4308 304C15 0.07x 18 8 - -
1.4303 - 305S19 305 S30500 - X5CrNi18-12 - - - 0.06x 18 11 - -
1.4305 - 303S31 303 S30300 58M X10CrNiS18-9 2346 - - 0.10x 18 8 - 0.35xS
1.4306 - - 304L - - X2CrNi19-11 2352 - - 0.030x 18 10 - -
1.4307 - 304S11 304L S30403 - - 2352 - 304C12 0.030x 18 8 - -
1.4310 - 301S21 301 S30100 - X12CrNi17-7 2331 - - .05/.15 17 6 - -
1.4311 - 304S61 304LN S30453 - X2CrNiN18-10 2371 1.4309 - 0.030x 18 9 - 0.22xN
1.4372 - - 201 S20100 - - - - - 0.15x 17 4.5 - 6.5Mn
1.4401 - 316S31 316 S31600 58J X5CrNiMo17-12-2 2347 1.4408 316C16 0.07x 17 11 2 -
1.4404 - 316S11 316L S31603 - X2CrNiMo17-13-2 2348 1.4409 316C12 0.030x 17 11 2 -
1.4406 - 316S61 316LN S31653 - X2CrNiMoN17-12-2 - - - 0.030x 17 11 2 0.22xN
1.4432 - 316S13 316L - - - 2353 - - 0.030x 17 11 2.5 -
1.4435 - 316S13 316L - - XCrNiMo18-14-3 2353 - - 0.030x 17 13 2.5 -
1.4436 - 316S33 316 - 58J X5CrNiMo17-13-3 2343 - - 0.05 17 11 2.5 -
1.4438 - 317S12 317L S31703 - - 2367 - - 0.030x 18 13 3 -
1.4439 - - - - - X2CrNiMoN17-13-5 - 1.4446 - 0.030x 17 13 4 0.22xN
1.4541 - 321S31 321 S32100 58B X6CrNiTi18-10 2337 - - 0.08x 18 9 - 0.5Ti
1.4550 - 347S31 347 S34700 58F X6CrNiNb18-10 2338 1.4552 347C17 0.08x 18 9 - 0.5Nb
1.4563 Sanicro28/Alloy28 - - N08028 - X1NiCrMoCu31-27-4 2584 - - 0.02x 26 30 3.0 1.0Cu
1.4567 - 394S17 304Cu S30430 - - - - - 0.04x 18 9 - 4xCu
1.4571 - 320S31 (316Ti) S31635 - X6CrNoMoTi17-12-2 2350 1.4581 - 0.08x 17 11 2 0.5Ti
1.4539 904L 904S13 - N08904 - X1CrNiMoCuN25-20-5 2562 1.4584 - 0.020x 19 24 4 1.5Cu
1.4547 254SMO/F44 - - S31254 - - 2378 1.4593 - 0.020x 20 18 6 0.75Cu
1.4529 1925hMo - - N08925 - X1NiCrMoCuN25-20-6 - 1.4588 - 0.020x 19 24 6 1.25Cu

Note
Composition Guide figures are intended to be representative of the grade, not typical.
'x' indicates a maximum

top

Office and Postal Address: BSSA, The Innovation Centre, 217 Portobello, Sheffield S1 4DP

Registered Office: Pegasus House, 463A Glossop Road, Sheffield S10 2QD

Tel: +44 (0)114 292 2636    |     Email: admin@bssa.org.uk

Copyright © 2018 British Stainless Steel Association

web design sheffield by Llama Digital