Ambient temperature mechanical properties for BS EN 10297-2 for stainless steel seamless tubes for general purposes
Steel grade | Delivery Condition | Proof strength min MPA | Tensile strength MPa |
Elongation A min % |
Resistance to intergranular corrosion | |||
Steel name | Steel number | Rp0.2 | Rp1.0 | Rm | long | trans | ||
Ferritic | ||||||||
X2CrTi12 | 1.4512 | +A | 210 | 220 | 380 | 25 | 25 | No |
X6CrAl13 | 1.4002 | +A | 210 | 220 | 400 | 17 | 17 | No |
X6Cr17 | 1.4016 | +A | 240 | 250 | 430 | 20 | 20 | Yes* |
X3CrTi17 | 1.4510 | +A | 230 | 240 | 420 | 23 | 23 | Yes |
Martensitic | ||||||||
X12Cr13 | 1.4006 | +QT 550 | 400 | 410 | 550 | 15 | 15 | No |
+QT 650 | 450 | 460 | 650 | 12 | 12 | No | ||
Austenitic | ||||||||
X2CrNi18-9 | 1.4307 | +AT | 180 | 215 | 460 | 40 | 35 | Yes |
X2CrNi19-11 | 1.4306 | +AT | 180 | 215 | 460 | 40 | 35 | Yes |
X2CrNiN18-10 | 1.4311 | +AT | 270 | 305 | 550 | 35 | 30 | Yes |
X5CrNi18-10 | 1.4301 | +AT | 195 | 230 | 500 | 40 | 35 | Yes* |
X8CrNiS18-9 | 1.4305 | +AT | 190 | 230 | 500 | 35 | 35 | No |
X6CrNiTi18-10 | 1.4541 | +AT (cold finished) | 200 | 235 | 500 | 35 | 30 | Yes |
+AT (hot finished) | 180 | 215 | 460 | 35 | 30 | Yes | ||
X6CrNiNb18-10 | 1.4550 | 205 | 240 | 510 | 35 | 30 | Yes | |
X1CrNi25-21 | 1.4335 | 180 | 210 | 470 | 45 | 40 | Yes | |
X2CrNiMo17-12-2 | 1.4404 | 190 | 225 | 490 | 40 | 30 | Yes | |
X5CrNiMo17-12-2 | 1.4401 | 205 | 240 | 510 | 40 | 30 | Yes* | |
X1CrNiMoN25-22-2 | 1.4466 | 260 | 295 | 540 | 40 | 30 | - | |
XCrNiMoTi17-12-2 | 1.4571 | +AT (cold finished) | 210 | 245 | 500 | 35 | 30 | Yes |
+AT (hot finished) | 190 | 225 | 490 | 35 | 30 | Yes | ||
X6CrNiMoNb17-12-3 | 1.4580 | +AT | 215 | 250 | 510 | 35 | 30 | Yes |
X2CrNiMoN17-13-3 | 1.4429 | +AT | 295 | 330 | 580 | 35 | 30 | Yes |
X3CrNiMo17-13-3 | 1.4436 | +AT | 205 | 240 | 510 | 40 | 30 | Yes* |
X2CrNiMo18-14-3 | 1.4435 | +AT | 190 | 225 | 490 | 40 | 35 | Yes |
X2CrNiMoN17-13-5 | 1.4439 | +AT | 285 | 315 | 580 | 35 | 30 | Yes |
X1NiCrMoCuCu31-27-4 | 1.4563 | +AT | 215 | 245 | 500 | 40 | 35 | Yes |
X1NiCrMoCu25-20-5 | 1.4539 | +AT | 230 | 250 | 520 | 35 | 30 | Yes |
X1CrNiMoCuN20-18-7 | 1.4547 | +AT | 300 | 340 | 650 | 35 | 30 | Yes |
X1NiCrMoCuN25-20-7 | 1.4529 | +AT | 270 | 310 | 600 | 35 | - | Yes |
X2NiCrAlTi32-20 | 1.4558 | +AT | 180 | 210 | 450 | 35 | - | - |
Austenitic ferritic steels | ||||||||
X2CrNiN23-4 | 1.4362 | +AT | 400 | 410 | 600 | 25 | 25 | Yes |
X3CrNiMoN27-5-2 | 1.4460 | +AT | 460 | 470 | 620 | 20 | - | Yes |
X2CrNiMoN29-7-2 | 1.4477 | +AT > 10mm | 550 | 560 | 750 | 25 | 25 | Yes |
+AT < 10mm | 650 | 660 | 800 | 25 | 25 | Yes | ||
X2CrNiMoN22-5-3 | 1.4462 | +AT | 450 | 460 | 640 | 22 | - | Yes |
X2CrNiMoCuN25-6-3 | 1.4507 | +AT | 500 | 510 | 700 | 20 | 20 | Yes |
X2CrNiMoN25-7-4 | 1.4410 | +AT | 550 | 640 | 800 | 20 | 20 | Yes |
X2CrNiMoCuWN25-7-4 | 1.4501 | +AT | 550 | 640 | 800 | 20 | 20 | Yes |
X2CrNiMoSi18-5-3 | 1.4424 | +AT | 480 | 490 | 700 | 30 | 30 | Yes |
Ferritic Heat resisting steels | ||||||||
X18CrN28 | 1.4749 | +A | 280 | - | 500 | 15 | 15 | N/A |
Austenitic Heat resisting steels | ||||||||
X8CrNiTi18-10 | 1.4878 | +AT | 190 | 230 | 500 | 40 | 40 | N/A |
X9CrNiSiNCe21-11-2 | 1.4835 | +AT | 310 | 350 | 650 | 37 | 40 | N/A |
X12CrNi23-13 | 1.4833 | +AT | 210 | 250 | 500 | 33 | 35 | N/A |
X8CrNi25-21 | 1.4845 | +AT | 210 | 250 | 500 | 33 | 35 | N/A |
X10NiCrAlTi32-21 | 1.4876 | +AT | 170 | 210 | 450 | 28 | 30 | N/A |
X6NiCrSiNCe35-25 | 1.4854 | +AT | 300 | 340 | 650 | 40 | 40 | N/A |