Chemical composition of stainless steels to BS 3605

Introduction

BS 3605 was published in two parts. Part 1 covered seamless pipes and tubes and part 2 covered welded pipes and tubes. All of these products were intended for pressure purpose applications.
The steel compositions were common to both parts of the standard, so are only shown once in the table in this article.
Both parts of BS 3605 are now withdrawn (as at March 2005). Part 1 has been replaced by BSEN 10216-5 and part 2 by BSEN 10217-7. The BS 3605 grade designations have not been used in the new European Standards but are shown in this article for historical interest.

As an alternative to scanning down the list try the 'find' facility on your keyboard, using the 'Ctrl' and 'F' keys together. Type in the term you are looking for in the dialog box that then appears.

The data given is not intended to replace that shown in individual standards to which reference should always be made.

BS 3605 chemical composition table

Grade
Chemical composition (% by mass - max unless stated)
- C Si Mn S P Cr Ni Mo Others
215S15 0.06/0.15 0.20/1.00 5.50/7.00 0.030 0.040 14.0/16.0 9.00/11.00 0.08/1.20 V 0.15/0.40:Nb 0.75/1.25:B 0.003/0.009
304S11 0.030 1.00 2.00 0.030 0.040 17.0/19.0 9.0/12.0 - -
304S31 0.070 1.00 2.00 0.030 0.040 17.0/19.0 8.0/11.0 - -
304S51 0.04/0.10 1.00 2.00 0.030 0.040 17.0/19.0 8.0/11.0 - -
316S11 0.030 1.00 2.00 0.030 0.040 16.5/18.5 11.0/14.0 2.00/2.50 -
316S13 0.030 1.00 2.00 0.030 0.040 16.5/18.5 11.5/14.5 2.50/3.00 -
316S31 0.070 1.00 2.00 0.030 0.040 16.5/18.5 10.5/13.5 2.00/2.50 -
316S33 0.070 1.00 2.00 0.030 0.040 16.5/18.5 11.0/14.0 2.50/3.00 -
316S51 0.04/0.10 1.00 2.00 0.030 0.040 16.5/18.5 10.5/13.5 2.00/2.50 -
316S52 0.04/0.10 1.00 2.00 0.030 0.040 16.5/18.5 10.5/13.5 2.00/2.50 B 0.0015/0.006
321S31 0.080 1.00 2.00 0.030 0.040 17.0/19.0 9.0/12.0 - Ti 5C/0.80
321S51 0.04/0.10 1.00 2.00 0.030 0.040 17.0/19.0 9.0/12.0 - Ti 5C/0.80
347S31 0.080 1.00 2.00 0.030 0.040 17.0/19.0 9.0/13.0 - Nb 10C/1.00
347S51 0.04/0.10 1.00 2.00 0.030 0.040 17.0/19.0 9.0/13.0 - Nb 10C/1.00

top

Office and Postal Address: BSSA, Regus, Blades Enterprise Centre, John Street, Sheffield S2 4SW

Registered Office: Pegasus House, 463A Glossop Road, Sheffield S10 2QD

Tel: +44 (0)114 292 2636    |     Email: admin@bssa.org.uk

Copyright © 2018 British Stainless Steel Association

web design sheffield by Llama Digital