Ambient temperature mechanical properties of martensitic and precipitation hardening stainless steel long products to BS EN 10088-3

Introduction

BS EN 10088-3 gives the mechanical properties for stainless steel semi-finished products, bars, rods and sections for general purposes. This article covers martensitic and precipitation hardening stainless steels. The properties given are proof strength, tensile strength, elongation and hardness.

The data given is not intended to replace that shown in individual standards to which reference should always be made.

BS EN 10088-3:20014 Edition

BS EN 10088-3 was originally published in 1995. The second version, BS EN 10088-3:2005, has been superseded by BS EN 10088-3:2014.

The tables shown here only have the 2014 tensile property ranges of the martensitic and precipitation hardening steels. Two new grades have been added, 1.4150 and 1.4612.

The mechanical properties of the following grades were changed:
1.4313, 1.4028, 1.4122, 1.4057, 1.4606.

This article does not include bright products.

BS EN 10088-3 mechanical properties - martensitic and precipitation hardening stainless steels

 

Designation Mechanical properties min unless stated
Steel name Steel number Thickness d mm Heat treatment condition1) Proof strength Rp0.2 3) N/mm2 Tensile strength R m 3) N/mm3 Elongation A3) % Max hardness2) HB
Martensitic stainless steels-standard grades
X12Cr13 1.4006 - A - max. 730 - 220
<160 QT650 450 650/850 15 -
X12CrS13 1.4005 - A - max. 730 - 220
<160 QT650 450 650/850 12 -
X15Cr13 1.4024 - A - max. 730 - 220
<160 QT650 450 650/850 15 -    
X20Cr13 1.4021 - A - max. 760 - 230
<160 QT700 500 700/850 13 -
<160 QT800 600 800/950 12 -
X30Cr13 1.4028 - A - max. 800 - 245
<160 QT850 650 850/1000 10 -
X39Cr13 1.4031 - A - max. 800 - 245
<160 QT800 650 800/1000 10 -
X46Cr13 1.4034 - A - max. 800 - 245
<160 QT800 650 850/1000 10 -
X38CrMo14 1.4419 - A - max. 760 - 235
X50CrMoV15 1.4116 - A - max. 900 - 280
X55CrMo14 1.4110 <100 A - max. 950 - 280
X14CrMoS17 1.4104 - A - max. 730 - 220
<60 QT650 500 650/850 12 -
60<160 QT650 500 650/850 10 -
X39CrMo17-1 1.4122 - A - max. 900 - 280
<60 QT750 550 750/950 12 -
60<160 QT750 550 750/950 12 -
X17CrNi16-2 1.4057 - A - max. 950 - 295
<60 QT800 600 800/950 14 -
60<160 QT800 600 800/950 12 -
<60 QT900 700 900/1050 12 -
60<160 QT900 700 900/1050 10 -
X3CrNiMo13-4 1.4313 - A - 1100 - 320
<160 QT700 520 700/850 15 -
160<250 QT700 520 700/850 12 -
<160 QT780 620 780/980 15 -
160<250 QT780 620 780/980 12 -
<160 QT900 800 900/1100 12 -
160<250 QT900 800 900/1100 10 -
X4CrNiMo16-5-1 1.4418 - A - 1100 - 320
<160 QT760 550 760/960 16 -
160<250 QT760 550 760/960 14 -
<160 QT900 700 900/1100 16 -
160<250 QT900 700 900/1100 14 -
Martensitic stainless steels-special grades
X29CrS13 1.4029 <160 A - max. 800 - 245
<160 QT850 650 850/1000 9 -
X46CrS13 1.4035 < 63 A - max. 800   245
X70CrMo15 1.4109 <100 A - max. 900 - 280
X40CrMoVN 1.4123 <100 A - - - 280
X105CrMo17 1.4125 <100 A - - - 285
X90CrMoV18 1.4112 <100 A - - - 265
X2CrNiMoV13-5-2 1.4415 <160 QT750 650 750/ 900 18 -
<160 QT850 750 850/1000 15 -
X53CrSiMoVN16-2 1.4150 <100 A - - - 255
QT - - - -
Precipitation hardening stainless steels-standard grades
X5CrNiCuNb16-4 1.4542 <100 AT - max. 1200 - 360
P800 520 800/950 18 -
P930 720 930/1100 16 -
P960 790 960/1160 12 -
P1070 1000 1070/1270 10 -
X7CrNiAl17-7 1.4568 <30 AT - max. 850 - 255
X5CrNiMoCuNb14-5 1.4594 <100 AT - max. 1200 - 360
P930 720 930/1100 15 -
P1000 860 1000/1200 10 -
P1070 1000 1070/1270 10 -
Precipitation hardening stainless steels-standard grades
X1CrNiMoAlTi12-9-2 1.4530 <150 AT - max.1200   363
P1200 1100 min. 1200 12  
 X1CrNiMoAlTi12-10-2 1.4596 < 150  AT - max 1200    363
P1400 1300 min 1400 9  
X1CrNiMoAlTi12-11-2 1.4612 < 150  AT - - - 331
P1510 1380 min 1510 10  
P1650 1515 min 1650 10  
X5NiCrTiMoVB25-15-2 1.4606 < 50 AT 250 max 700 35 212
P880 550 880/1150 20  


Note

  1. A= annealed; QT=quenched and tempered.
  2. Only for guidance.
  3. for rods, only the tensile strength values apply.
  4. Note 4 deleted

 

top

Office and Postal Address: BSSA, Regus, Blades Enterprise Centre, John Street, Sheffield S2 4SW

Registered Office: Pegasus House, 463A Glossop Road, Sheffield S10 2QD

Tel: +44 (0)114 292 2636    |     Email: admin@bssa.org.uk

Copyright © 2017 British Stainless Steel Association