Availability of Stainless Steel Grades
Availability of Stainless Steel Products
The tables below give an indication of the availability of stainless steel flat and long products. The intention is to give designers and specifiers some idea of how easy it will be to source their choice of grade and product form. The information has been created as a response to enquiries for rare grades which are difficult to source in small quantities.
Comments are invited on the tables. It is likely with such a large amount of information that there are some differences of opinion about the availability of some grades. If you want to make a comment on this table please email to ssas@bssa.org.uk or call 0114 2671265.
Availability of Flat Products Grades from EN 10088-2
The table below contains all grades listed in EN 10088-2. The meaning of the availability scores is:
1 - Readily available from any recognised stainless steel stockholder
2 - Available from a significant number of specialist stainless steel stockholders
3 - Available from a limited number of suppliers
4 - Available only from stainless steel mills if sufficient quantity required
5 - Not practically available
N/A - Not applicable - Indicates that the grade is not intended to be made in that product form. For example, most ferritic grades would not be made as plate.
| EN Designation |
Alternative Designations |
Availability |
| Steel name |
Steel number |
AISI |
UNS |
Other US |
BS |
Generic/Brand
|
Plate |
Sheet |
| Ferritic stainless steels - standard grades |
| X2CrNi12 |
1.4003 |
|
S40977 |
|
|
3CR12 |
2 |
2 |
| X2CrTi12 |
1.4512 |
409 |
S40900 |
|
409S19 |
|
N/A |
2 |
| X6CrNiTi12 |
1.4516 |
|
|
|
|
|
N/A |
4 |
| X6Cr13 |
1.4000 |
410S |
S41008 |
|
403S17 |
|
3 |
3 |
| X6CrAl13 |
1.4002 |
405 |
S40500 |
|
405S17 |
|
4 |
4 |
| X6Cr17 |
1.4016 |
430 |
S43000 |
|
430S17 |
|
N/A |
1 |
| X3CrTi17 |
1.4510 |
439 |
S43035 |
|
|
|
N/A |
2 |
| X3CrNb17 |
1.4511 |
430Nb |
|
|
|
|
N/A |
4 |
| X6CrMo17-1 |
1.4113 |
434 |
S43400 |
|
434S17 |
|
N/A |
4 |
| X2CrMoTi18-2 |
1.4521 |
444 |
S44400 |
|
|
|
N/A |
3 |
| Ferritic stainless steels - special grades |
| X2CrTi17 |
1.4520 |
|
|
|
|
|
N/A |
4 |
| X1CrNb15 |
1.4595 |
|
|
|
|
|
N/A |
4 |
| X2CrMoTi17-1 |
1.4513 |
|
|
|
|
|
N/A |
4 |
| X6CrNi17-1 |
1.4017 |
|
|
|
|
|
N/A |
4 |
| X5CrNiMoTi15-2 |
1.4589 |
|
S42035 |
|
|
|
N/A |
4 |
| X6CrMoNb17-1 |
1.4526 |
436 |
S43600 |
|
|
|
N/A |
3 |
| X2CrNbZr17 |
1.4590 |
|
|
|
|
|
N/A |
4 |
| X2CrTiNb18 |
1.4509 |
441 |
S43932 |
|
|
18CrCb |
N/A |
2 |
| X2CrMoTi29-4 |
1.4592 |
|
S44700 |
|
|
29-4 |
N/A |
4 |
| Ferritic stainless steels - heat resisting grades |
| X10CrAlSi7 |
1.4713 |
|
|
|
|
|
3 |
3 |
| X10CrAlSi13 |
1.4724 |
|
|
|
|
|
3 |
3 |
| X10CrAlSi18 |
1.4742 |
|
|
|
|
|
3 |
3 |
| X18CrN28 |
1.4749 |
446 |
|
|
|
|
3 |
3 |
| X10CrAlSi25 |
1.4762 |
|
|
|
|
|
3 |
3 |
| Martensitic stainless steels - standard grades |
| X12Cr13 |
1.4006 |
410 |
S41000 |
|
410S21 |
|
3 |
3 |
| X15Cr13 |
1.4024 |
420 |
S42000 |
|
|
|
3 |
3 |
| X20Cr13 |
1.4021 |
420 |
S42000 |
|
420S29 |
|
3 |
3 |
| X30Cr13 |
1.4028 |
420 |
S42000 |
|
420S45 |
|
3 |
3 |
| X39Cr13 |
1.4031 |
420 |
S42000 |
|
420S45 |
|
3 |
3 |
| X46Cr13 |
1.4034 |
420 |
S42000 |
|
|
|
3 |
3 |
| X38CrMo14 |
1.4419 |
|
|
|
|
|
5 |
5 |
| X55CrMo14 |
1.4110 |
|
|
|
|
|
5 |
5 |
| X50CrMoV15 |
1.4116 |
|
|
|
|
|
4 |
4 |
| X39CrMo17-1 |
1.4122 |
|
|
|
|
|
5 |
5 |
| X3CrNiMo13-4 |
1.4313 |
|
S41500 |
F6NM |
|
|
3 |
3 |
| X4CrNiMo16-5-1 |
1.4418 |
|
|
|
|
248 SV |
3 |
3 |
| Martensitic and precipitation-hardening steels - special grades |
| X1CrNiMoCu12-5-2 |
1.4422 |
|
|
|
|
|
5 |
5 |
| X1CrNiMoCu12-7-3 |
1.4423 |
|
|
|
|
|
5 |
5 |
| X5CrNiCuNb16-4 |
1.4542 |
|
S17400 |
|
|
17-4 PH |
3 |
3 |
| X7CrNiAl17-7 |
1.4568 |
|
S17700 |
|
|
17-7 PH |
N/A |
2 |
| Austenitic stainless steels - standard grades |
| X10CrNi18-8 |
1.4310 |
301 |
S30100 |
|
301S21 |
|
N/A |
2 |
| X2CrNiN18-7 |
1.4318 |
301LN |
S30153 |
|
|
|
N/A |
3 |
| X2CrNi18-9 |
1.4307 |
304L |
S30403 |
|
304S11 |
|
1 |
1 |
| X2CrNi19-11 |
1.4306 |
304L |
S30403 |
|
|
|
4 |
4 |
| X2CrNiN18-10 |
1.4311 |
304LN |
S30453 |
|
304S51 |
|
3 |
4 |
| X5CrNi18-10 |
1.4301 |
304 |
S30400 |
|
304S15 |
|
1 |
1 |
| X8CrNiS18-9 |
1.4305 |
303 |
S30300 |
|
303S31 |
|
3 |
N/A |
| X6CrNiTi18-10 |
1.4541 |
321 |
S32100 |
|
321S31 |
|
2 |
2 |
| X4CrNi18-12 |
1.4303 |
305 |
S30500 |
|
305S19 |
|
N/A |
4 |
| X2CrNiMo17-12-2 |
1.4404 |
316L |
S31603 |
|
316S11 |
|
1 |
1 |
| X2CrNiMoN17-11-2 |
1.4406 |
316LN |
S31653 |
|
316S61 |
|
4 |
4 |
| X5CrNiMo17-12-2 |
1.4401 |
316 |
S31600 |
|
316S31 |
|
1 |
1 |
| X6CrNiMoTi17-12-2 |
1.4571 |
316Ti |
S31635 |
|
320S31 |
|
3 |
3 |
| X2CrNiMo17-12-3 |
1.4432 |
316L |
S31603 |
|
316S13 |
|
2 |
3 |
| X2CrNiMo18-14-3 |
1.4435 |
316L |
S31603 |
|
316S13 |
|
4 |
4 |
| X2CrNiMoN17-13-5 |
1.4439 |
317LMN |
|
|
|
|
4 |
4 |
| X1NiCrMoCu25-20-5 |
1.4539 |
|
N08904 |
|
904S13 |
904L |
3 |
3 |
| Austenitic stainless steels - special grades |
| X5CrNi17-7 |
1.4319 |
|
|
|
|
|
4 |
4 |
| X5CrNiN19-9 |
1.4315 |
|
|
|
|
|
4 |
4 |
| X1CrNi25-21 |
1.4335 |
310L |
|
|
|
|
4 |
4 |
| X6CrNiNb18-10 |
1.4550 |
347 |
S34700 |
|
347S31 |
|
4 |
3 |
| X1CrNiMoN25-22-2 |
1.4466 |
310MoLN |
S31050 |
|
|
|
4 |
4 |
| X6CrNiMoNb17-12-2 |
1.4580 |
|
|
|
|
|
5 |
5 |
| X2CrNiMoN17-3-3 |
1.4429 |
316LN |
S31653 |
|
|
|
4 |
4 |
| X3CrNiMo17-13-3 |
1.4436 |
316 |
S31600 |
|
316S33 |
|
3 |
3 |
| X2CrNiMoN18-12-4 |
1.4434 |
317LN |
S31753 |
|
|
|
4 |
4 |
| X2CrNiMo18-15-4 |
1.4438 |
317L |
|
|
317S12 |
|
4 |
4 |
| X1CrNiMoCuN24-22-8 |
1.4652 |
|
|
|
|
|
4 |
4 |
| X1CrNiSi18-15-4 |
1.4361 |
|
|
|
|
|
4 |
4 |
| X11CrNiMnN19-8-6 |
1.4369 |
|
|
|
|
|
4 |
3 |
| X12CrMnNiN17-7-5 |
1.4372 |
201 |
S20100 |
|
|
|
4 |
3 |
| X2CrMnNiN17-7-5 |
1.4371 |
201L |
S20103 |
|
|
|
4 |
3 |
| X12CrMnNiN18-9-5 |
1.4373 |
202 |
S20200 |
|
|
|
4 |
3 |
| X9CrMnCuNB17-8-3 |
1.4597 |
204Cu |
S20430 |
|
|
|
N/A |
3 |
| X1NiCrMo31-27-4 |
1.4563 |
|
N08028 |
|
|
Sanicro 28 |
4 |
4 |
| X1CrNiMoCuN25-25-5 |
1.4537 |
|
|
|
|
|
5 |
5 |
| X1CrNiMoCuN20-18-7 |
1.4547 |
|
S31254 |
F44 |
|
254SMO |
3 |
3 |
| X1CrNiMoCuNW24-22-6 |
1.4659 |
|
|
|
|
|
4 |
4 |
| X1NiCrMoCuN25-20-7 |
1.4529 |
|
N08925 |
|
|
1925hMo |
3 |
3 |
| X2CrNiMnMoN25-18-6-5 |
1.4565 |
|
|
|
|
|
3 |
N/A |
| X9CrMnNiCu 17-8-5-2 |
1.4618 |
|
|
|
|
|
4 |
4 |
| |
1.3964 |
|
|
|
|
XM-19 |
3 |
N/A |
| Austenitic stainless steels - heat resisting grades |
| X8CrNiTi18-10 |
1.4878 |
321 |
S32100 |
|
|
|
3 |
3 |
| X15CrNiSi20-12 |
1.4828 |
|
|
|
|
|
3 |
3 |
| X9CrNiSiNCe21-11-2 |
1.4835 |
|
S30815 |
|
|
253 MA |
3 |
3 |
| X12CrNi23-13 |
1.4833 |
309 |
S30900 |
|
309S24 |
|
3 |
3 |
| X8CrNi25-21 |
1.4845 |
310S |
S31000 |
|
310S24 |
|
2 |
2 |
| X15CrNiSi25-21 |
1.4841 |
314 |
S31400 |
|
|
|
4 |
4 |
| X6CrNiSiNCe19-10 |
1.4818 |
|
S30415 |
|
|
153 MA |
4 |
4 |
| X10NiCrSi35-19 |
1.4886 |
|
|
|
|
330 |
3 |
3 |
| Austenitic stainless steels - creep resisting grades |
| X6CrNi18-10 |
1.4948 |
304H |
S30409 |
|
304S51 |
|
3 |
4 |
| X6CrNiMoB17-12-2 |
1.4919 |
316H |
S31635 |
|
316S51 |
|
3 |
4 |
| Austenitic-ferritic stainless steels-standard grades |
| X2CrNiN22-2 |
1.4062 |
|
S32202 |
|
|
|
4 |
4 |
| X2CrMnNiN21-5-1 |
1.4162 |
|
S32101 |
|
|
2101 LDX |
3 |
3 |
| X2CrNiN23-4 |
1.4362 |
|
S32304 |
|
|
2304 |
3 |
3 |
| X2CrNiMoN12-5-3 |
1.4462 |
|
S31803/
S32205
|
F51 |
|
2205 |
2 |
2 |
| Austenitic-ferritic stainless steels-special grades |
| X2CrNiCuN23-4 |
1.4655 |
|
|
|
|
|
5 |
5 |
| X2CrNiMoN29-7-2 |
1.4477 |
|
|
|
|
|
5 |
5 |
| X2CrNiMoCuN25-6-3 |
1.4507 |
|
|
F61 |
|
Ferrinox 255 |
3 |
3 |
| X2CrNiMoN25-7-4 |
1.4410 |
|
S32750 |
F53 |
|
2507 |
2 |
3 |
| X2CrNiMoCuWN25-7-4 |
1.4501 |
|
S32760 |
F55 |
|
Zeron 100 |
2 |
3 |
| X2CrNiMoSi18-5-3 |
1.4424 |
|
|
|
|
|
5 |
5 |
Availability of Long Products Grades from EN 10088-3
The table below contains all grades listed in EN 10088-3. The meaning of the availability scores is:
1 - Readily available from any recognised stainless steel stockholder
2 - Available from a significant number of specialist stainless steel stockholders
3 - Available from a limited number of suppliers
4 - Available only from stainless steel mills if sufficient quantity required
5 - Not practically available
N/A - Not applicable - Indicates that the grade is not intended to be made in that product form. For example, most ferritic grades would not be made as plate.
The table below contains all grades listed in EN 10088-3. In addition, there are some grades not in the current edition but which are expected to be in future editions. Some heat resisting steels from EN 10095 and creep resisting steels from EN 10302 are also included.
| EN Designation |
Alternative designation |
Availability |
| Steel name |
Steel number |
AISI |
UNS |
Other US |
BS |
Generic/Brand |
Bar |
Wire |
| Ferritic stainless steels-standard grades |
| X2CrNi12 |
1.4003 |
|
S40977 |
|
|
|
3 |
4 |
| X6Cr13 |
1.4000 |
410S |
S41008 |
|
403S17 |
|
3 |
3 |
| X6Cr17 |
1.4016 |
430 |
S43000 |
|
430S17 |
|
2 |
2 |
| X6CrMoS17 |
1.4105 |
|
|
|
|
|
2 |
2 |
| X6CrMo17-1 |
1.4113 |
434 |
S43400 |
|
|
|
3 |
3 |
| Ferritic stainless steels-special grades |
| X2CrTi17 |
1.4520 |
|
|
|
|
|
4 |
4 |
| X3CrNb17 |
1.4511 |
|
|
|
|
|
4 |
4 |
| X2CrMoTiS18-2 4 |
1.4523 |
|
|
|
|
|
4 |
4 |
| X6CrMoNb17-1 |
1.4526 |
436 |
S43600 |
|
|
|
4 |
4 |
| X2CrTiNb18 |
1.4509 |
441 |
S43932 |
|
|
18CrCb |
4 |
4 |
| Ferritic stainless stees - Heat resisting grades |
| X10CrAlSi7 |
1.4713 |
|
|
|
|
|
3 |
3 |
| X10CrAlSi18 |
1.4742 |
|
|
|
|
|
4 |
4 |
| X10CrAlSi25 |
1.4762 |
|
|
|
|
|
4 |
4 |
| Martensitic stainless steels-standard grades |
| X12Cr13 |
1.4006 |
410 |
S41000 |
|
|
|
2 |
2 |
| X12CrS13 |
1.4005 |
416 |
S41600 |
|
|
|
2 |
2 |
| X20Cr13 |
1.4021 |
420 |
S42000 |
|
420S29 |
|
2 |
2 |
| X30Cr13 |
1.4028 |
420 |
S42000 |
|
420S45 |
|
2 |
2 |
| X39Cr13 |
1.4031 |
420 |
S42000 |
|
420S45 |
|
3 |
3 |
| X46Cr13 |
1.4034 |
420 |
S42000 |
|
|
|
3 |
3 |
| X38CrMo14 |
1.4419 |
|
|
|
|
|
4 |
4 |
| X50CrMoV15 |
1.4116 |
|
|
|
|
|
3 |
3 |
| X55CrMo14 |
1.4110 |
|
|
|
|
|
4 |
4 |
| X14CrMoS17 |
1.4104 |
|
|
|
|
|
2 |
2 |
| X39CrMo17-1 |
1.4122 |
|
|
|
|
|
2 |
N/A |
| X17CrNi16-2 |
1.4057 |
431 |
S43100 |
|
431S29 |
|
1 |
N/A |
| X3CrNiMo13-4 |
1.4313 |
|
S41500 |
F6NM |
|
|
3 |
N/A |
| X4CrNiMo16-5-1 |
1.4418 |
|
|
|
|
248SV |
3 |
N/A |
| Martensitic stainless steels-special grades |
| X29CrS13 |
1.4029 |
|
|
|
|
|
4 |
4 |
| X46CrS13 |
1.4035 |
|
|
|
|
|
4 |
4 |
| X70CrMo15 |
1.4109 |
|
|
|
|
|
3 |
4 |
| X40CrMoVN16-2 |
1.4123 |
|
|
|
|
|
4 |
4 |
| X105CrMo17 |
1.4125 |
440C |
S44004 |
|
|
|
3 |
N/A |
| X90CrMoV18 |
1.4112 |
440B |
S44003 |
|
|
|
3 |
N/A |
| X2CrNiMoV13-5-2 |
1.4415 |
|
|
|
|
|
4 |
4 |
| Martensitic stainless steels-creep resisting grades |
| X20CrMoV11-1 |
1.4922 |
|
|
|
|
|
3 |
N/A |
| X22CrMoV12-1 |
1.4923 |
|
|
|
|
|
3 |
N/A |
| Precipitation hardening stainless steels-standard grades |
| X5CrNiCuNb16-4 |
1.4542 |
|
S17400 |
|
|
17-4 PH |
2 |
3 |
| X7CrNiAl17-7 |
1.4568 |
|
S17700 |
|
|
17-7 PH |
N/A |
3 |
| X5CrNiMoCuNb14-5 |
1.4594 |
|
|
|
|
FV 520B |
3 |
N/A |
| Precipitation hardening stainless steels-special grades |
| X1CrNiMoAlTi12-9-2 |
1.4530 |
|
|
|
|
|
4 |
N/A |
| X1CrNiMoAlTi12-10-2 |
1.4596 |
|
|
|
|
|
4 |
N/A |
| X5NiCrTiMoVB25-12-2 |
1.4606 |
|
|
|
|
|
4 |
N/A |
| Austenitic stainless steels-standard grades |
| X10CrNi18-8 |
1.4310 |
301 |
S30100 |
|
301S21 |
|
N/A |
1 |
| X2CrNi18-9 |
1.4307 |
304L |
S30403 |
|
304S11 |
|
1 |
1 |
| X2CrNi19-11 |
1.4306 |
304L |
S30403 |
|
304S11 |
|
3 |
3 |
| X2CrNiN18-10 |
1.4311 |
304LN |
S30453 |
|
304S61 |
|
3 |
3 |
| X5CrNi18-10 |
1.4301 |
304 |
S30400 |
|
304S31 |
|
1 |
1 |
| X8CrNiS18-9 |
1.4305 |
303 |
S30300 |
|
303S31 |
|
1 |
1 |
| X6CrNiTi18-10 |
1.4541 |
321 |
S32100 |
|
321S31 |
|
2 |
2 |
| X4CrNi18-12 |
1.4303 |
305 |
S30500 |
|
|
|
4 |
4 |
| X2CrNiMo17-12-2 |
1.4404 |
|
S31603 |
|
316S11 |
|
1 |
1 |
| X2CrNiMoN17-11-2 |
1.4406 |
316LN |
S31653 |
|
|
|
4 |
4 |
| X5CrMo17-12-2 |
1.4401 |
316 |
S31600 |
|
316S31 |
|
1 |
1 |
| X6CrNiMoTi17-12-2 |
1.4571 |
316Ti |
S31635 |
|
320S31 |
|
2 |
2 |
| X2CrNiMo17-12-3 |
1.4432 |
316L |
S31603 |
|
316S13 |
|
4 |
4 |
| X2CrNiMoN17-13-3 |
1.4429 |
316LN |
S31653 |
|
|
|
3 |
4 |
| X3CrNiMo17-13-3 |
1.4436 |
316 |
S31600 |
|
316S33 |
|
3 |
3 |
| X2CrNiMo18-14-3 |
1.4435 |
316L |
S31603 |
|
|
|
3 |
3 |
| X2CrNiMoN17-13-5 |
1.4439 |
317LMN |
S31726 |
|
|
|
4 |
4 |
| X6CrNiCuS18-9-2 |
1.4570 |
|
|
|
|
|
3 |
3 |
| X3CrNiCu18-9-4 |
1.4567 |
304Cu |
S30430 |
|
394S17 |
|
2 |
2 |
| X1NiCrMoCu25-20-5 |
1.4539 |
904L |
N09804 |
|
904S13 |
|
2 |
2 |
| Austenitic stainless steels-special grades |
| X5CrNi17-7 |
1.4319 |
302 |
S30200 |
|
302S25 |
|
4 |
2 |
| X9CrNi18-9 |
1.4325 |
|
|
|
|
|
4 |
4 |
| X5CrNiN19-9 |
1.4315 |
304N |
S30451 |
|
|
|
4 |
4 |
| X6CrNiNb18-10 |
1.4550 |
347 |
S34700 |
|
347S31 |
|
3 |
4 |
| X1CrNiMoN25-22-2 |
1.4466 |
310MoLN |
S31050 |
|
|
|
4 |
4 |
| X6CrNiMoNb17-12-2 |
1.4580 |
316Cb |
S31640 |
|
|
|
4 |
4 |
| X2CrNiMo18-15-4 |
1.4438 |
317L |
S31703 |
|
317S12 |
|
4 |
4 |
| X1CrNiMoCuN24-22-8 |
1.4652 |
S32654 |
|
|
|
654SMO |
4 |
4 |
| X1CrNiSi18-15-4 |
1.4361 |
306 |
S30600 |
|
|
|
4 |
4 |
| X11CrNiMnN19-8-6 |
1.4369 |
|
|
|
|
|
4 |
4 |
| X12CrMnNiN17-7-5 |
1.4372 |
201 |
S20100 |
|
|
|
3 |
3 |
| X8CrMnNiN18-9-5 |
1.4374 |
|
|
|
|
|
4 |
4 |
| X8CrMnCuNB17-8-3 |
1.4597 |
S20430 |
|
|
|
|
3 |
3 |
| X3CrNiCu19-9-2 |
1.4560 |
|
|
|
|
|
4 |
4 |
| X3CrNiCuMo17-11-3-2 |
1.4578 |
|
|
|
|
|
4 |
4 |
| X1NiCrMoCu31-27-4 |
1.4563 |
|
N08028 |
|
|
Sanicro 28 |
3 |
3 |
| X1CrNiMoCuN25-25-5 |
1.4537 |
|
N08932 |
|
|
|
4 |
4 |
| X1CrNiMoCuN20-18-7 4 |
1.4547 |
|
S31254 |
|
|
254 SMO |
3 |
3 |
| X2CrNiMoCuS17-10-2 |
1.4598 |
|
|
|
|
|
3 |
4 |
| X1CrNiMoCuNW24-22-6 |
1.4659 |
|
S31266 |
|
|
|
4 |
4 |
| X1NiCrMoCuN25-20-7 |
1.4529 |
|
N08925 |
|
|
1925hMo |
3 |
3 |
| X2CrNiMnMoN25-18-6-5 |
1.4565 |
|
S34565 |
|
|
|
3 |
4 |
| X2CrNiMnmoNNb21-16-5-3 |
1.3964 |
|
S20910 |
|
|
Nitronic 50 |
3 |
3 |
| |
|
|
S21800 |
|
|
Nitronic 60 |
3 |
3 |
| Austenitic stainless steels - Heat resisting steels |
| X6CrNiSiNCe19-10 |
1.4818 |
|
S30415 |
|
|
|
4 |
4 |
| X15CrNiSi20-12 |
1.4828 |
309Si |
|
|
|
|
3 |
3 |
| X12CrNi23-13 |
1.4833 |
309 |
S30900 |
|
309S16 |
|
3 |
3 |
| X9CrNiSiNCe21-11-2 |
1.4835 |
|
S30815 |
|
|
253 MA |
3 |
3 |
| X8CrNi25-21 |
1.4845 |
310S |
S31008 |
|
310S31 |
|
2 |
2 |
| X15CrNiSi25-21 |
1.4841 |
314 |
S31400 |
|
|
|
2 |
2 |
| X12NiCrSi35-16 |
1.4864 |
|
|
|
|
|
4 |
3 |
| X10NiCrSi35-19 |
1.4886 |
330 |
N08330 |
|
|
|
3 |
3 |
| Austenitic stainless steels - Creep resisting grades |
| X6CrNiMoB17-12-2 |
1.4919 |
316H |
S31609 |
|
|
|
4 |
4 |
| X6CrNi18-10 |
1.4948 |
304H |
S30409 |
|
|
|
3 |
3 |
| X6NiCrTiMoVB25-15-2 |
1.4980 |
|
S66286 |
|
|
A286 |
3 |
4 |
| Austenitic-ferritic stainless steels-Standard grades |
| X2CrNiN22-2 |
1.4062 |
|
S32202 |
|
|
DX 2202 |
3 |
3 |
| X2CrMnNiN21-5-1 |
1.4162 |
|
S32101 |
|
|
2101 LDX |
2 |
2 |
| X3CrNiMoN27-5-2 |
1.4460 |
329 |
S31260 |
|
|
|
3 |
N/A |
| X2CrNiMoN22-5-3 |
1.4462 |
|
S31803/
S32205
|
|
|
2205 |
2 |
2 |
| Austenitic-ferritic stainless steels-special grades |
| X2CrNiN23-4 |
1.4362 |
|
S32304 |
|
|
2304 |
3 |
3 |
| X2CrNiMoN29-7-2 4 |
1.4477 |
|
|
|
|
|
4 |
4 |
| X2CrNiMoCuN25-6-3 |
1.4507 |
|
S32550 |
|
|
Ferrinox 255 |
2 |
2 |
| X2CrNiMoN25-7-4 4 |
1.4410 |
|
S32750 |
|
|
2507 |
2 |
2 |
| X2CrNiMoCuWN25-7-4 |
1.4501 |
|
S32760 |
|
|
Zeron 100 |
2 |
3 |
| X2CrNiMoSi18-5-3 |
1.4424 |
|
S31500 |
|
|
|
4 |
4 |
top
Follow us on Twitter