Ambient temperature mechanical properties of heat resisting steels to BS EN 10095

Introduction

BS EN 10095 is the material standard for heat resisting steels and nickel alloys. Mechanical properties (proof strength, tensile strength, hardness and elongation) of the common grades of stainless steel covered in the standard are listed. Ferritic, austenitic and austenitic-ferritic (duplex) grades are included.

The data given is not intended to replace that shown in individual standards to which reference should always be made.

BS EN 10095 mechanical properties tables

Designation HB max. 1)2)3) Proof Strength Tensile Strength Rm N/mm2 A % min.
Name Number Rp0.2 N/mm2 min. 3) Rp1.0 N/mm2 min. 3)
Ferritic heat-resisting steels
X10CrAlSi13 1.4724 192 250 - 450/650 15
X10CrAlSi18 1.4742 212 270 - 500/700 15
X10CrAlSi25 1.4762 223 280 - 520/720 15
X18CrN28 1.4749 212 280 - 500/700 15
X3CrAlTi18-2 1.4736 200 280 - 500/650 25
Austenitic heat-resisting steels
X8CrNiTi18-10 1.4878 215 190 230 500/720 401)
X15CrNiSi20-12 1.4828 223 230 270 550/750 301)
X9CrNiSiNCe21-11-2 1.4835 210 310 350 650/850 401)
X12CrNi23-13 1.4833 192 210 250 500/700 351)
X8CrNi25-21 1.4845 192 210 250 500/700 351)
X15CrNiSi25-21 1.4841 223 230 270 550/750 301)
X12NiCrSi35-16 1.4864 223 230 270 550/750 301)
X10NiCrAlTi32-21 1.4876 192 170 210 450/680 301)
X6NiCrNbCe32-27 1.4877 223 180 220 500/750 351)
X25CrMnNiN25-9-7 1.4872 311 500 540 850/1 050 251)
X6CrNiSiNCe19-10 1.4818 210 290 330 600/800 401)
X6NiCrSiNCe35-25 1.4854 210 300 340 650/850 401)
X10NiCrSi35-19 1.4886 200 270 300 500/650 40
X10NiCrSiNb35-22 1.4887 200 270 300 500/650 40
Austenitic-ferritic heat-resisting steel
X15CrNiSi25-4 1.4821 235 400 - 600/850 16
1)The maximum HB values may be raised by 100 units or the maximum tensile strength value may be raised by 200 N/mm2 and the minimum elongation value be lowered to 20% for sections and bars of < 35 mm thickness having a final cold deformation.
2) For guidance only.
3)For rods, only the tensile strength values apply.

top

Office and Postal Address: BSSA, Regus, Blades Enterprise Centre, John Street, Sheffield S2 4SW

Registered Office: Pegasus House, 463A Glossop Road, Sheffield S10 2QD

Tel: +44 (0)114 292 2636    |     Email: admin@bssa.org.uk

Copyright © 2017 British Stainless Steel Association

web design sheffield by Llama Digital