Mechanical properties for stainless steels to BS EN 10217-7

Introduction

BS EN 10217-7 2005 is the material standard for stainless steels for welded tubes for pressure purposes. This new standard was first published in February 2005.

As an alternative to scanning down the list try the 'find' facility on your keyboard, using the 'Ctrl' and 'F' keys together. Type in the term you are looking for in the dialog box that then appears.
The data given is not intended to replace that shown in individual standards to which reference should always be made.

BS EN 10217-7 mechanical property tables 

Tensile and Impact Properties
   Tensile properties at RT Impact properties
Steel grade Proof Strength                         Tensile strength Elongation Minimum average of 3 Charpy (J)
  Rp0.2 Rp1.0 Rm A min (%) at RT  at -sub-zero temperature1
Steel name Steel number MPa MPa MPa long trans long trans trans
Austenitic steels
X2CrNi18-9 1.4307 180 215 470-670 40 35 100 60 60
X2CrNi19-11 1.4306 180 215 460-680 40 35 100 60 60
X2CrNiN18-10 1.4311 270 305 550-760 35 30 100 60 60
X5CrNi18-10 1.4301 195 230 500-700 40 35 100 60 60
X6CrNiTi18-10 1.4541 200  235 500-730 35 30 100  60 60
X6CrNiNb18-10 1.4550 205 240 510-740 35 30 100  60 60
X2CrNiMo17-12-2 1.4404 190 225 490-690 40 30 100 60 60
X5CrNiMo17-12-2 1.4401 205 240 510-710 40 30 100 60 60
XCrNiMoTi17-12-2 1.4571 210 245 500-730 35 30 100 60 60
X2CrNiMo17-12-3 1.4432 190 225 490-690 40 30 100 60 60
X2CrNiMoN17-13-3 1.4429 295 330 580-800 35 30 100 60   60 
X3CrNiMo17-13-3 1.4436 205 240 510-710 40 30 100 60   60 
X2CrNiMo18-14-3 1.4435 190 225 490-690 40 30 100 60   60  
X2CrNiMoN17-13-5 1.4439 285 315 580-800 35 30 100 60   60  
X2CrNiMo18-15-4 1.4438 220 250 490-690 35 30 100 60 60
X1NiCrMoCu31-27-4 1.4563 215 245 500-750 40 35 120 90 60
X1CrNiMoCu25-20-5 1.4539 220 250 520-720 35 30 120  90 60
X1CrNiMoCuN20-18-7 1.4547 300 340  650-850  35 30 100  60 60
X1NiCrMoCuN25-20-7 1.4529 300 340 600-800 40 40 120 90 60
Duplex - Austenitic ferritic steels
X2CrNiN23-4 1.4362 400 ----  600-820  25 25 120  90 40
X2CrNiMoN22-5-3 1.4462 450 ----  700-920  25  20 120 90 40
X2CrNiMoN25-7-4 1.4410 550 ---- 800-1000  20 20 100  100 40
X2CrNiMoCuWN25-7-4 1.4501 550 ---- 800-1000 20 20 100 100 40

1.For austenitic steels the sub-zero test temperature is -196 deg C. For duplex steels it is - 40 deg C.

Elevated temperature 0.2 %proof strength values for austenitic steels
Steel grade Rp0.2 min MPa at a temperature of (deg C)                              
Steel name                   Steel number 50 100 150 200 250 300 350 400 450 500 550
X2CrNi18-9 1.4307 165 147 132  118  108  100  94  89  85  81 80 
X2CrNi19-11 1.4306 165 147  132  118  108  100  94 89 85  81  80 
X2CrNiN18-10 1.4311 255 205  175  157  145  136  130  125  121  119  118 
X5CrNi18-10 1.4301 180 157  142  127  118  110  104  98 95 92  90 
X6CrNiTi18-10 1.4541 190 176  167  157  147 136  130  125  121  119  118
X6CrNiNb18-10 1.4550 195 177  167  157  147  136 130  125  121 119  118 
X2CrNiMo17-12-2 1.4404 182 166  152  137  127  118  113  108  103  100  98 
X5CrNiMo17-12-2 1.4401 193 177  162  147  137  127  120  115  112  110  108 
XCrNiMoTi17-12-2 1.4571 202 185  177  167  157  145  140  135  131  129  127 
X2CrNiMo17-12-3 1.4432 182 166 152 137  127  118  113  108  103  100  98 
X2CrNiMoN17-13-3 1.4429 260 211  185  167  155 145  140  135  131  129  127 
X3CrNiMo17-13-3 1.4436 195 177  162  147  137  127  120  115  112  110  108 
X2CrNiMo18-14-3 1.4435 180  165  150  137  127  119  113  108  103  100  98 
X2CrNiMoN17-13-5 1.4439 260 225 200  185  175  165  155  150    ---    ---   ---
X2CrNiMo18-15-4 1.4438 200 172  157  147  137  127  120  115  112  110  108 
X1NiCrMoCu31-27-4 1.4563 210 190  175  160  155  150  145  135  125  120  115 
X1CrNiMoCu25-20-5 1.4539 216 205 190  175  160  145  135  125  115  110  105 
X1CrNiMoCuN20-18-7 1.4547 267 230  205  190  180  170  165  160  153  148    ---
X2CrNiMoCuWN25-7-4 1.4529 270 230  210  190  180  170  165  160  130  120  105 

Elevated temperature 1.0% proof strength values for austenitic steels
Steel grade Rp1.0 min MPa at a temperature of (deg C)                              
Steel name                   Steel number 50 100 150 200 250 300 350 400 450 500 550
X2CrNi18-9 1.4307 200 181 162  147  137 127 121 116 112  109 108 
X2CrNi19-11 1.4306 200 181 162 147 137 127 121 116 112 109 108
X2CrNiN18-10 1.4311 282 240 210 187  175  167  161 156  152 149  147 
X5CrNi18-10 1.4301 218 191  172  157  145  135  129 125 122 120 120
X6CrNiTi18-10 1.4541 222 208 196 186  177 167  161 156  152  149  147
X6CrNiNb18-10 1.4550 232 211  196 186  177  167 161  156  152 149  147 
X2CrNiMo17-12-2 1.4404 217 199 181  167  157  145  139  135  130  128 127 
X5CrNiMo17-12-2 1.4401 230 211  191  177  167  156  150  144 141  139  137
XCrNiMoTi17-12-2 1.4571 232 218  206  196 186  175  169  164  160  158  157 
X2CrNiMo17-12-3 1.4432 217 199 181 167  157  145  139  135  130  128  127 
X2CrNiMoN17-13-3 1.4429 290 246  218  198  183 175  169 164 160 158  157 
X3CrNiMo17-13-3 1.4436 228 211 191  177  167  156  150  144  141  139 137
X2CrNiMo18-14-3 1.4435 217  200  180  165  153  145  139  135  130  128  127 
X2CrNiMoN17-13-5 1.4439 290 255 230  210 200  190  180  175    ---    ---   ---
X2CrNiMo18-15-4 1.4438 232 206  188  177  167  156  148  144  140  138 136
X1NiCrMoCu31-27-4 1.4563 240 220  205  190  185  180  175  165  155  150  145 
X1CrNiMoCu25-20-5 1.4539 244 235 220  205 190  175  165  155  145  140  135 
X1CrNiMoCuN20-18-7 1.4547 306 270  245  225 212  200 195  190  184  180    ---
X2CrNiMoCuWN25-7-4 1.4529 310 270  245  225 215  205  195  190  160  150  135 

top

Office and Postal Address: BSSA, Regus, Blades Enterprise Centre, John Street, Sheffield S2 4SW

Registered Office: Pegasus House, 463A Glossop Road, Sheffield S10 2QD

Tel: +44 (0)114 292 2636    |     Email: admin@bssa.org.uk

Copyright © 2017 British Stainless Steel Association

web design sheffield by Llama Digital