Chemical composition of stainless steels to BS 1449-2

Introduction

BS 1449-2 Specification for stainless and heat-resisting steel plate, sheet and strip was last published in 1983. It covered flat products in both annealed and temper (cold) rolled supply conditions.
The standard was withdrawn in 1999 following the publication of BS EN 10088-2 in 1995 (stainless grades) and BS EN 10095 (heat-resisting grades) in 1995. BS 1449-2 should not be used for specifying new products, but may still be included in specifications for products originally designed before 1995 and so is included here for reference purposes only. Flat products for pressure purposes are now covered by BS EN 10028-7.

As an alternative to scanning down the list try the 'find' facility on your keyboard, using the 'Ctrl' and 'F' keys together. Type in the term you are looking for in the dialog box that then appears.

The data given is not intended to replace that shown in individual standards to which reference should always be made.

BS 1449-2 chemical composition table

Grade
Chemical composition (% by mass - max unless stated)
- C Si Mn S P Cr Ni Mo Others
Austenitic steels
284S16 0.07 1.00 7.00/10.0 0.030 0.060 16.5/18.5 4.00/6.50 - N 0.15/0.25
301S21 0.15 1.00 2.00 0.030 0.045 16.0/18.0 6.0/8.0 - -
304S11 0.030 1.00 2.00 0.030 0.045 17.0/19.0 9.0/12.0 - -
304S15 0.06 1.00 2.00 0.030 0.045 17.5/19.0 8.0/11.0 - -
304S16 0.06 1.00 2.00 0.030 0.045 17.5/19.0 9.0/11.0 - -
304S31 0.07 1.00 2.00 0.030 0.045 17.0/19.0 8.0/11.0 - -
305S19 0.10 1.00 2.00 0.030 0.045 17.0/19.0 11.0/13.0 - -
309S24 0.15 1.00 2.00 0.030 0.045 22.0/25.0 13.0/16.0 - -
310S24 0.15 1.00 2.50 0.030 0.045 23.0/26.0 19.0/22.0 - -
315S16 0.07 1.00 2.00 0.030 0.045 16.5/18.5 9.0/11.0 1.25/1.75 -
316S11 0.030 1.00 2.00 0.030 0.045 16.5/18.5 11.0/14.0 2.0/2.5 -
316S13 0.030 1.00 2.00 0.030 0.045 16.5/18.5 11.5/14.5 2.5/3.0 -
316S31 0.07 1.00 2.00 0.030 0.045 16.5/18.5 10.5/13.5 2.0/2.5 -
316S33 0.07 1.00 2.00 0.030 0.045 16.5/18.5 11.0/14.0 2.5/3.0 -
317S12 0.03 1.00 2.00 0.030 0.045 17.5/19.5 14.0/17.0 3.0/4.0 -
317S16 0.06 1.00 2.00 0.030 0.045 17.5/19.5 12.0/15.0 3.0/4.0 -
320S31 0.08 1.00 2.00 0.030 0.045 16.5/18.5 11.0/14.0 2.0/2.5 Ti 5C/0.80
320S33 0.08 1.00 2.00 0.030 0.045 16.5/18.5 11.5/14.5 2.5/3.0 Ti 5C/0.80
321S31 0.08 1.00 2.00 0.030 0.045 17.0/19.0 9.0/12.0 - Ti 5C/0.80
347S31 0.08 1.00 2.00 0.030 0.045 17.0/19.0 9.0/12.0 - Nb 10C/1.00
Ferritic steels
403S17 0.08 1.00 1.00 0.030 0.040 12.0/14.0 1.00 - -
405S17 0.08 1.00 1.00 0.030 0.040 12.0/14.0 1.00 - Al 0.10/0.30
409S19 0.08 1.00 1.00 0.030 0.040 10.5/12.5 1.00 - Ti 6C/1.0
430S17 0.08 1.00 1.00 0.030 0.040 16.0/18.0 1.00 - -
434S17 0.08 1.00 1.00 0.030 0.040 16.0/18.0 1.00 0.90/1.30 -
Martensitic steels
410S21 0.09/0.15 1.00 1.00 0.030 0.040 11.5/13.5 1.00 - -
420S45 0.28/0.36 1.00 1.00 0.030 0.040 12.0/14.0 1.00 - -

top

British Stainless Steel Association (BSSA): registered in England and Wales as a private company limited by guarantee; registration no. 07547349

Registered Office: Broomgrove, 59 Clarkehouse Road, Sheffield S10 2LE, United Kingdom

Tel: +44 (0)114 267 1260    |     Fax: +44 (0)114 266 1252     |     Email: enquiry@bssa.org.uk

Copyright © 2007-2012 British Stainless Steel Association

web design sheffield by Llama Digital   |   Businessmagnet IAP Partner