Chemical composition of stainless steel castings to BS EN 10283

Introduction

BS EN 10283 is the material standard for stainless steel castings for corrosion resisting purposes. Martensitic, precipitation hardening, austenitic and austenitic-ferritic (duplex) grades are included. The chemical composition of all the grades of stainless steel covered in the standard are listed.

As an alternative to scanning down the list try the 'find' facility on your keyboard, using the 'Ctrl' and 'F' keys together. Type in the term you are looking for in the dialog box that then appears.

The data given is not intended to replace that shown in individual standards to which reference should always be made.

BS EN 10283 chemical composition table

 
Designation Chemical composition % by mass (max unless otherwise stated)
Steel name Steel number C Si Mn P S Cr Mo Ni N Cu Nb1) W V
Martensitic grades
GX12Cr12 1.4011 0.15 1.00 1.00 0.035 0.025 11.50/13.50 0.50 1.00 - 0.30 - - 0.08
GX7CrNiMo12-1 1.4008 0.10 1.00 1.00 0.035 0.025 12.00/13.50 0.20/0.50 1.00/2.00 - 0.30 - - 0.08
GX4CrNi13-4 1.4317 0.06 1.00 1.00 0.035 0.025 12.00/13.50 0.70 3.50/5.00 - 0.30 - - 0.08
GX4CrNiMo16-5-1 1.4405 0.06 0.80 1.00 0.035 0.025 15.00/17.00 0.70/1.50 4.00/6.00 - 0.30 - - 0.08
GX4CrNiMo16-5-2 1.4411 0.06 0.80 1.00 0.035 0.025 15.00/17.00 1.50/2.00 4.00/6.00 - 0.30 - - 0.08
GX5CrNiCu16-4 1.4525 0.07 0.80 1.00 0.035 0.025 15.00/17.00 0.80 3.50/5.50 0.05 2.50/4.00 0.35 - 0.08
Austenitic grades
GX2CrNi19-11 1.4309 0.030 1.50 2.00 0.035 0.025 18.00/20.00 - 9.00/12.00 0.20 0.50 - - -
GX5CrNi19-10 1.4308 0.07 1.50 1.50 0.040 0.030 18.00/20.00 - 8.00/11.00 - 0.50 - - -
GX5CrNiNb19-11 1.4552 0.07 1.50 1.50 0.040 0.030 18.00/20.00 - 9.00/12.00 - 0.50 8xC/1.00 - -
GX2CrNiMo19-11-2 1.4409 0.030 1.50 2.00 0.035 0.025 18.00/20.00 2.00/2.50 9.00/12.00 0.20 0.50 - - -
GX5CrNiMo19-11-2 1.4408 0.07 1.50 1.50 0.040 0.030 18.00/20.00 2.00/2.50 9.00/12.00 - 0.50 - - -
GX5CrNiMoNb19-11-2 1.4581 0.07 1.50 1.50 0.040 0.030 18.00/20.00 2.00/2.50 9.00/12.00 - 0.50 8xC/1.00 - -
GX5CrNiMo19-11-3 1.4412 0.07 1.50 1.50 0.040 0.030 18.00/20.00 3.00/3.50 10.00/13.00 - 0.50 - - -
GX2CrNiMoN17-13-4 1.4446 0.030 1.00 1.50 0.040 0.030 16.50/18.50 4.00/4.50 12.50/14.50 0.12/0.22 0.50 - - -
Fully austenitic grades
GX2NiCrMo28-20-2 1.4458 0.030 1.00 2.00 0.035 0.025 19.00/22.00 2.00/2.50 26.00/30.00 0.20 2.00 - - -
GX4NiCrCuMo30-20-4 1.4527 0.06 1.50 1.50 0.040 0.030 19.00/22.00 2.00/3.00 27.50/30.50 - 3.00/4.00 - - -
GX2NiCrMoCu25-20-5 1.4584 0.025 1.00 2.00 0.035 0.020 19.00/21.00 4.00/5.00 24.00/26.00 0.20 1.00/3.00 - - -
GX2NiCrMoN25-20-5 1.4416 0.030 1.00 1.00 0.035 0.020 19.00/21.00 4.50/5.50 24.00/26.00 0.12/0.20 0.50 - - -
GX2NiCrMoCuN29-25-5 1.4587 0.030 1.00 2.00 0.035 0.025 24.00/26.00 4.00/5.00 28.00/30.00 0.15/0.25 2.00/3.00 - - -
GX2NiCrMoCuN25-20-6 1.4588 0.025 1.00 2.00 0.035 0.020 19.00/21.00 6.00/7.00 24.00/26.00 0.10/0.25 0.50/1.50 - - -
GX2CrNiMoCuN20-18-6 1.4593 0.025 1.00 1.20 0.030 0.010 19.50/20.50 6.00/7.00 17.50/19.50 0.18/0.24 0.50/1.00 - - -
Austenitic-ferritic grades
GX6CrNiN26-7 1.4347 0.08 1.50 1.50 0.035 0.020 25.00/27.00 - 5.50/7.50 0.10/0.20 0.50 - - -
GX2CrNiMoN22-5-3 1.4470 0.030 1.00 2.00 0.035 0.025 21.00/23.00 2.50/3.50 4.50/6.50 0.12/0.20 0.50 - - -
GX2CrNiMoN25-6-3 1.4468 0.030 1.00 2.00 0.035 0.025 24.50/26.50 2.50/3.50 5.50/7.00 0.12/0.25 0.50 - - -
GX2CrNiMoCuN25-6-3-3 1.4517 0.030 1.00 1.50 0.035 0.025 24.50/26.50 2.50/3.50 5.00/7.00 0.12/0.22 2.75/3.50 - - -
GX2CrNiMoN25-7-3 1.4417 0.030 1.00 1.50 0.030 0.020 24.00/26.00 3.00/4.00 6.00/8.50 0.15/0.25 1.00 - 1.00 -
GX2CrNiMoN26-7-4 1.4469 0.030 1.00 1.00 0.035 0.025 25.00/27.00 3.00/5.00 6.00/8.00 0.12/0.22 1.30 - - -

Note 1 The niobium content value applies for the sum of the niobium + tantalum.

top

Office and Postal Address: BSSA, Regus, Blades Enterprise Centre, John Street, Sheffield S2 4SW

Registered Office: Pegasus House, 463A Glossop Road, Sheffield S10 2QD

Tel: +44 (0)114 292 2636    |     Fax: +44 (0)114 292 2633     |     Email: admin@bssa.org.uk

Copyright © 2017 British Stainless Steel Association

web design sheffield by Llama Digital